A123 capacity and internal resistance

The 3 cells are now assembled into a pack, which will speed up testing compared to doing each individually.

6 cycles have been performed on the pack so far, and the performance has been consistently around 19Ah. On cycle 3 the pack was accidentally over discharged, causing a temporary reduction in capacity that appears to be recovering over several cycles.

Cycle  Capacity    Notes
1      19.25Ah
2      19.22Ah    
3      19.20Ah     1
4      18.28Ah
5      19.00Ah
6      19.10Ah

Notes
1. Accidentally overdischarged to <1Vpc on cell 1. Ah value includes discharge only to 2.5Vpc

The cell internal resistance averages 2.5mOhm with some spread over time and cell that’s measured. The load was varied from 20A to 36A and voltage deltas used to calculate the internal resistance. X axis on the graph below is Ah discharged from full charge.

IR test 1

Test Setup
2014-05-19_18-59-18_704

Graphs:
Pack Cycle 1

Pack Cycle 2

Pack Cycle 3

Pack Cycle 3 charge

Pack Cycle 4

Pack Cycle 5

Pack Cycle 6

Raw data: A123 Battery Data

Leave a Reply